CostKit

Injection Molding Defect Checklist

A trial report that says "sink marks, flash" and a supplier who says "we'll tune it" can both be right, or both be stalling. This table orders 12 common defects by what to check first, so you can tell a two-hour setup change from a mold rework or a design change.

Twelve common defects

DefectCheck firstUsual root causeFixCost impact
Sink marks Section thickness above 4 mm, ribs too heavy Short packing, gate froze early, thick zone Longer hold, bigger gate, thin the thick area Settings only; thickness changes mean a mold change
Flash Clamp force vs projected area Low clamp force, worn parting line, melt too hot Raise clamp, rework parting line, drop melt temp Mold repair plus downtime
Silver streaks Resin dried, no degradation smell Moisture, overheated melt, injection too fast Dry 2–4 h, lower melt temp, slow the shot Nearly free — always check first
Warpage Cooling balance, ejection balance Uneven cooling, excessive packing, ejected too early Rework water lines, cool longer, balance ejection Often a mold change; the costliest defect
Short shot Injection pressure and gate size Low pressure, cold melt, poor venting More pressure/speed, larger gate, add vents Mostly settings
Burn marks Vent locations and injection speed Trapped gas, too fast at end of fill Cut vents, slow the final stage Small mold work
Weld lines Gate position and flow fronts Multiple gates meeting, cold melt or mold Raise mold/melt temp, move the gate Cosmetic parts usually need a mold change
Ejector marks Ejection force and draft angle Ejected too early, low draft, no release agent Cool longer, add draft, redistribute ejector pins Mold work plus polishing
Flow marks Injection speed and gate size Slow fill, small gate, cold mold Faster fill, bigger gate, warmer mold Mostly settings
Voids / bubbles Wall thickness core, moisture Shrink voids in thick walls, gas, low back pressure More back pressure, dry resin, thin the wall Thick parts usually need a design change
Colour streaks / black specks Purge before the run, masterbatch dispersion Incomplete purging, carbonised material on the screw Purge, pull the screw, change masterbatch Downtime plus scrap
Sticking / scuffing Draft angle and mold surface Insufficient draft, scored cavity, high packing Polish, add draft, reduce packing Mold work plus polishing

Troubleshooting order: material, then mold, then settings

On the floor the order is usually reversed: adjust settings first, blame the mold second, check the material last. It should be the other way round — rule out the resin, confirm the mold condition, and only then touch settings.

  1. Material: was it dried (ABS 80 °C for 2–3 h, PC 120 °C for 4 h), is it the right grade, is the masterbatch ratio right, is regrind too high? More than half of silver streaks, voids and black specks are material problems — no amount of tuning fixes them.
  2. Mold: crushed parting line, blocked vents, restricted water lines, off-centre ejector pins, worn gate. Flash, burn marks, ejector marks and sticking usually leave evidence here.
  3. Settings: melt and mold temperature, injection speed, packing, cooling time. Sink marks, short shots, flow marks and weld lines mostly live in this layer — and it is the layer people keep returning to, because settings suppress symptoms while the cause sits upstream.

Which defects are design problems

Suppliers do not volunteer a mold-rework quote for something a setup change can fix. The test is simple: does the defect follow the wall thickness, the gate, or the ejector pins?

Conversely, flash, silver streaks, flow marks and short shots are strongly tied to the current shot. Ask for a setup adjustment before agreeing to a rework quote: a mold change costs thousands and buys a week of tuning.

How defects become money

There are three cost layers, and quotations usually price only the first:

Put all three into the yield and secondary-operation fields of the molding cost calculator to get a real should-cost. Many "overpriced quote" arguments are really a supplier pricing these layers while the buyer compared resin and machine time only.

Three things to demand when discussing defects

  1. A first-article inspection report, not "we checked it". Key dimensions with measured values, not OK/NG.
  2. Trial parameter records: melt temp, mold temp, injection speed, packing, cooling. An undocumented adjustment cannot be reproduced and will return with the next lot of resin.
  3. An agreed cosmetic standard: which face, what size, how many are acceptable per part, written into the drawing or a limit sample. "It doesn't affect function" is the most expensive sentence in the conversation.

For cosmetic parts, define A, B and C surfaces at sampling stage. Otherwise every production lot reopens the same argument about whether a mark counts as a defect.

FAQ

Can more packing eliminate sink marks?

No. Packing only feeds shrinkage while the gate is still open; once it freezes, a thick section has nowhere to draw from. ABS sections over 4 mm will sink, and the cures are thinning, gas assist or a structural change.

Does flash always mean a mold change?

No. Check clamp force against projected area times cavity pressure, then inspect the parting line. Insufficient clamp force is a setup issue; a crushed parting line is a repair. Ask for the clamp force calculation before approving rework.

Why do silver streaks appear when we change resin lot?

The new lot usually differs in moisture content, or regrind share went up. Measure moisture first (above 0.2% is high for ABS), then consider degradation in the barrel.

Related: molding cost calculator · cycle time calculator · mold cost estimator · process selection guide · glossary