Surface Finishing Parameters
A drawing says "anodize 20 µm" and most buyers check the number, not what it does: bores close by 10 µm and corrosion life changes. The ranges for four processes sit below.
Thickness, cure temperature and salt spray hours move with substrate, bath and line discipline. The ranges below are a starting point, not a clause in a standard; the references cover how classes are designated and how the test is run.
1. Anodizing: half the film grows outward, half into the metal
Anodizing converts the substrate itself: at 20 µm about half grows inward, so each mating surface moves 10 µm and an M3 tapped hole with 5 µm of tolerance left stops the line. Hard anodizing prices at about twice decorative work, ¥25/dm² against ¥12/dm² in the finishing cost calculator.
| Type and thickness | Typical use | Neutral salt spray reference | Outside the range |
|---|---|---|---|
| Decorative 5 µm | Indoor nameplates, hidden parts | 24–48 h | Dye looks blotchy when the film is thin, and one assembly scratch reaches bare metal. 5 µm will not survive fingerprints and sweat |
| Decorative 10 µm | Consumer electronics housings, indoor structures | 96–200 h | The usual choice. Dropping to 5 µm saves very little, and one cosmetic rework costs more than the difference |
| Decorative 15 µm | Outdoor enclosures, light fittings | 240–480 h | Each surface grows 7.5 µm, so M3 tapped holes need allowance or the go gauge will not pass |
| Decorative 20–25 µm | Outdoor architectural parts, coastal sites | 500–1000 h | Each surface grows 10–12.5 µm. Interference fits and precision bores must be resized before the drawing is released |
| Hard anodizing 25–50 µm | Guide rails, cylinder bores, wear faces | 500 h+ at the same thickness | The film is brittle: sharp edges and fillets chip. Fatigue strength drops, so be careful with cyclic-load parts |
2. Powder and paint: the upper limit bites harder
Powder fails at the top of the range: above 120 µm curing stress stays in the film and the coat lifts as one sheet, the edge so clean it looks like missing pre-treatment. Cure time starts at part temperature, not at the oven door.
| Process and thickness | Cure schedule | Pre-treatment | Outside the range |
|---|---|---|---|
| Powder coating 60–80 µm | 180–200 °C, 10–20 min after the part reaches temperature | Phosphate or zirconium conversion, degreased | Thinner than this will not hide sanding marks; above 120 µm the film cracks and lifts as one sheet under impact |
| Outdoor polyester powder 80–120 µm | As above | Zinc phosphating, 1–3 g/m² | Below this range on coastal or humid sites, chalking starts within two years |
| Wet paint 20–40 µm | Air dry, or 60–80 °C for 30 min | Degrease, sand, primer | One heavy coat blisters and pin-holes. Too thin and sanding scratches show through, and rework means full stripping |
| E-coat 15–25 µm | 160–180 °C for 20–30 min | Zinc phosphating | Excess voltage gives uneven thickness, and internal cavities and welds show bare metal first |
| Second pass over an existing coat | Another 180–200 °C bake | Old film must be fully stripped | Two stacked films lose adhesion fast: cross-hatch testing lifts flakes, and it costs more than a new part |
3. Plating: thickness sets corrosion life, not the hours
The salt spray test fixes conditions only, 5% sodium chloride at 35 °C, which is what ASTM B117 covers. "Must pass 96 hours" comes from the drawing, and whether white rust counts as failure halves the number.
| Deposit and thickness | Purpose | Neutral salt spray reference | Outside the range |
|---|---|---|---|
| Zinc 8–12 µm | General steel corrosion protection | 24–96 h (white to red rust) | Below 8 µm red rust appears within 24 h. Too thick and the deposit turns brittle, with hydrogen embrittlement risk on high-strength parts |
| Zinc-nickel 8–12 µm | Automotive fasteners, high salt spray demand | 720–1000 h | Costs three to four times zinc plating. On indoor parts that money buys nothing |
| Nickel 10–25 µm | Decorative finish and wear underlayer | 96–200 h | A thin nickel layer is porous, and pitting starts at the pores in the steel below |
| Decorative chromium 0.1–0.5 µm | Top coat for gloss and wear | Counted with the nickel layer | Too thin and the nickel shows through as a yellow cast. Too thick and internal stress cracks the deposit at bends |
| Electroless nickel 10–25 µm | Complex cavities needing uniform thickness | 200–500 h | As the bath ages the phosphorus content drifts, and corrosion resistance varies across the same batch |
| Tin 5–10 µm | Solderability on electronics | 24–48 h | Below this, solderability fades quickly. Parts stored six months need a fresh solderability test |
4. Pre-treatment and masking: money cut here returns as rework
Cutting degreasing from ten minutes to three saves cents a part and lifts cratering from 2% to 15%. Masking trades the same way: an unmasked thread is chased by hand, two minutes on an M6.
| Step | Parameters | Acceptance | Cost of getting it wrong |
|---|---|---|---|
| Alkaline degreasing | 50–60 °C, 5–10 min, pH 9–11 | Water film stays unbroken for 30 s | Incomplete degreasing gives cratering across the whole powder coat, and the only fix is stripping everything |
| Pickling | Ambient, 5–15 min, pull out when bubbling stops | Avoid over-pickling | Over-pickled steel blackens, plating adhesion drops, and the deposit lifts when the part is bent |
| Blasting | Sa 2½, roughness Ra 3–6 µm | Reach pre-treatment within 4 h | Too smooth and adhesion is weak; too rough and a thin coat cannot cover the peaks |
| Phosphating | 1–3 g/m² coating weight, fine crystal | No smut, no rust spots | Smut left behind kills adhesion, and salt spray blistering starts exactly there |
| Masking (threads, bores, mating faces) | 0.3–1 min of hand work per point | High-temperature tape or silicone plugs, seated with no gap | One missed thread means chasing it by hand afterwards, and that hour costs ten times the masking |
| Racking | 20–60 parts per rack, contacts on non-cosmetic faces | Good electrical contact at every point | Poor contact leaves bare patches. Rack marks are the most common defect on plated parts |
How the parameters reach the cost
- Thickness class sets the price band. Going from 10 µm to 20 µm anodizing adds roughly 30% in chemicals and power. In the finishing cost calculator that is a move up from ¥12/dm². If the part only needs fingerprint resistance indoors, the extra money is paid on every piece.
- Rework rate sets the real cost. A quoted unit price is a good-part price; rework is billed as a whole part. At 15% cratering the effective price is about 1.18 times the quote, which outweighs any chemistry increase.
- Masking and racking set the labour. Both are per part. On small lots this line is larger than the chemistry and only thins out at volume. The rate side is covered in machine hour rate.
Machining and sheet metal comparisons are in the machining cost and sheet metal cost pages, trade-offs in the process selection guide.
Six numbers to ask for on a quotation
- The minimum thickness and where it is measured (per-surface minimum, or an average)
- Salt spray hours and the failure criterion (white or red rust, part or coupon)
- Pre-treatment type (phosphate, zirconium, blasting) with coating weight or roughness
- Cure temperature and when the clock starts (door or part temperature)
- Number of masking points and how they are masked, and whether they are included
- Rework rules: who pays for cratering, bare patches and colour mismatch
The first two decide acceptance, the last four the invoice. Terms are in the glossary.
Four common mistakes
- Treating film thickness as pure addition. An anodic film grows half inward, so 20 µm moves the surface by about 10 µm. That reasoning does not transfer to powder: 80 µm is 80 µm, and every hole shrinks by 160 µm across.
- Reading salt spray hours as a warranty. B117 fixes the test conditions, not the line. The same thickness from different batches can differ threefold. Acceptance needs a coupon that went through the bath with the parts, not a verbal promise.
- Plating the mating faces to save masking time. Deposit thickness varies across the part, so the assembly either will not go together or the layer flakes when pressed. Masking is cheaper than the assembly line.
- Ignoring hydrogen embrittlement. High-strength steel and springs that skip the bake can fail weeks later with no visible corrosion at the fracture. If the bake is not on the quotation, ask for it.
FAQ
10 µm or 20 µm anodizing?
Indoors 10 µm is enough, outdoors starts at 15 µm, coastal sites want 20 µm or more; a tight aluminium housing should go to 15 µm with the holes pre-opened.
References
- Anodizing of aluminium and its alloys — decorative and protective anodic oxidation coatings ISO · ISO 7599
- Operating salt spray (fog) apparatus ASTM · ASTM B117
Basis for the parameters above. Links go to the publisher or its search page; the standard text itself is sold by the publisher. Price references are public market ranges, not supplier quotations.