Die Casting Process Parameters
Quotes rarely stall because the arithmetic is wrong; they stall because nobody knows what parameters the part should be run at. This page puts the four parameter families side by side — shot speed, intensification pressure, temperature, timing — each with a working range and the defects you get outside it, so a trial report saying "cold shuts" or "porosity" can be read as "the profile is not dialled in" or "the die cannot do this".
Ranges move with alloy, wall thickness and machine. The values below are common starting points in the industry, not clauses of a standard; the final numbers come from a documented trial. The references at the foot of the page cover defect acceptance and dimensional tolerances — they are not the basis for the speeds and pressures above.
1. Shot speed: two stages plus a gate velocity
The shot profile has two stages: slow shot pushes metal through the sleeve and expels sleeve air, fast shot fills the cavity in tens of milliseconds. Between them sits a conversion — plunger speed and gate velocity are linked by the area ratio, so "how fast did we open the plunger" means nothing until it is converted to the gate.
| Parameter | Working range | What it does | Outside the range | How to set it |
|---|---|---|---|---|
| Slow shot speed (plunger) | 0.1–0.5 m/s | Pushes the metal through the shot sleeve and expels sleeve air before the gate seals | Too high: air entrapment and folded oxide skin — subsurface porosity; too low: the metal front cools, cold shuts and misruns | Slower when sleeve fill is low; start from 0.2 m/s |
| Fast-shot position (share of sleeve length) | 70%–90% of the sleeve | Decides when the profile switches to high speed | Too early: sleeve air is pushed into the cavity before it can escape; too late: metal is already past the gate at slow speed and the far end chills | Set it where the metal front just reaches the gate |
| Fast shot speed (plunger) | 1–6 m/s | Sets gate velocity and fill time — the most sensitive line on the shot curve | Too high: washout, soldering, sprayed and entrapped metal; too low: flow marks, cold shuts, misruns | Fix gate velocity first, then back-calculate plunger speed |
| Gate velocity | Al 30–60 m/s; Zn 30–50; Mg 40–70; Cu 20–40 | Sets the fill pattern: too low and the cavity does not fill, too high and the stream atomises and curls air in | Too high: die washout, aluminium pickup, porosity; too low: misruns, flow marks, cold shuts | v gate = v plunger × (plunger area ÷ gate area) |
| Fill time | 20–100 ms (depends on weight and wall) | From first metal entering the cavity to full — the only test of whether venting can keep up | Too long: cold shuts, misruns; too short: gas cannot escape, porosity and blisters | Short for thin large parts, longer for heavy sections; size overflows and vents first |
Excess gate velocity is the classic case of tuning that makes things worse: the die face washes out, the crater changes the fill direction, porosity moves with it, and every adjustment behaves like a different part. Check the "washout / soldering" row in the die casting defect checklist before touching the profile again.
2. Intensification pressure: range by alloy, upper half by wall
Intensification pressure — the metal pressure acting on the projected area after intensification — decides whether shrinkage porosity can be squeezed shut. For one alloy, go to the top of the range when walls are thin, flow length is long, or the part must be pressure-tight; but clamp force rises with it, and a machine that is too small will flash. The tonnage and sleeve fill calculator converts pressure into clamp force, so the two pages must use the same value.
| Alloy | Typical range | Preset on this site | Below the range | Above the range |
|---|---|---|---|---|
| Zinc (Zn) | 20–40 MPa | 40 MPa | Shrinkage porosity, sinks, rough surface | Flash, sticking, faster die wear |
| Aluminium (Al) | 40–90 MPa | 60 MPa (normal walls) / 80 MPa (thin, large) / 90 MPa (pressure-tight) | Shrinkage porosity, failed pressure test | Flash, washout, ejection problems |
| Magnesium (Mg) | 40–60 MPa | 50 MPa | Shrinkage porosity, hot tears | Flash, hot tears, higher die thermal load |
| Copper (Cu) | 60–100 MPa | No preset — enter by alloy and wall | Shrinkage porosity, misruns | Extreme die thermal load, very short die life |
3. Temperature: pouring sets fluidity, die temperature sets the fill
The two do different jobs. Pouring temperature sets how fluid the metal is; die temperature sets how fast it cools once inside. Both low gives cold shuts; both high gives sticking and gas pickup — so "raise every temperature" is not a general fix. Work out which end is short first.
| Alloy | Pouring temperature | Die temperature | Pouring too cold | Die too hot |
|---|---|---|---|---|
| Zinc (Zn) | 400–430 °C | 150–200 °C | Cold shuts, misruns | Sticking, sinks, longer cooling |
| Aluminium (Al) | 650–700 °C | 180–260 °C | Cold shuts, misruns | Sticking, more gas pickup (more porosity) |
| Magnesium (Mg) | 630–680 °C | 200–260 °C | Cold shuts, cracking | More oxidation, sticking |
| Copper (Cu) | 900–1000 °C | 250–350 °C | Cold shuts, misruns | Faster thermal fatigue, die life collapses |
Die temperature is not available at start-up: in continuous running the die heats itself from the castings, so the first few dozen shots are cold. That is the usual reason a trial report and a production report disagree. What matters for stability is the heat-balanced die temperature, not shot one.
4. Timing: build-up, dwell, spray
These three times go straight into the cycle, and the cycle is machine cost. Two extra seconds of dwell on a 30-second cycle is over 6% of machine time; but squeezing dwell out and getting distortion and ejection cracks costs far more than that 6%.
| Parameter | Working range | What it does | What drifting costs |
|---|---|---|---|
| Intensification build-up time | 10–30 ms | From a full cavity to final intensification pressure | Too long: shrinkage porosity, cold shuts; too short: flash, shock loading on the die and shot end |
| Dwell time | 3–10 s (set by the thickest section) | Lets the casting gain enough strength before ejection | Too short: distortion, ejection cracks, sticking; too long: sticking, scoring, longer cycle — machine time climbs directly |
| Spray and blow-off | 1–3 s per shot | Release and die temperature control; also decides whether the die face builds up | Too much coating: blisters and porosity; too little: sticking and scoring |
| Die temperature stability | Within the alloy range, ±10 °C | Keeps the fill pattern and solidification order stable | Large swings: lot-to-lot drift in dimensions and defects, settings become unreproducible |
Why these ranges are only a starting point
Die casting needs several conditions to hold at once: the same settings on another machine behave differently because tonnage, shot capacity, sleeve diameter and shot-end condition all differ; the same machine with a different share of returns behaves differently again because gas content and fluidity move. Treating the ranges as an acceptance standard is guaranteed to start an argument.
Use them as a question list instead. Faced with a trial report, ask for slow shot speed, fast-shot position, the gate velocity and the area used to convert it, intensification pressure, die temperature, and dwell time. A supplier who cannot answer those usually cannot hold consistency in production either.
How parameters become cost
- Cycle → machine time: fill time is tens of milliseconds and irrelevant; dwell, spray, blow-off, open/close and extraction make up most of the cycle. Going from 6 s to 9 s of dwell on a 30-second cycle adds about 10%, and it lands on the machine-time line of the die casting cost calculator.
- Pressure and speed → die life: sustained high gate velocity and pressure at the top of the range accelerate thermal fatigue and washout. Dropping from 100,000 to 60,000 shots raises cost per shot by 67% — the mould cost estimator prices that directly.
- Spray and die temperature → yield: heavy coating blisters, die temperature swings drift lot to lot. Going from 95% to 88% yield multiplies unit cost by 1/(1−p), about 8%, and that belongs in the yield field of the calculator.
In other words, parameters are not an internal shop-floor matter: they set machine time, tooling amortisation and yield at the same time. In a negotiation, "this part is difficult" can be tested by asking for the numbers in the tables above and seeing which one genuinely leaves the range.
The eight numbers to request at a trial
- Alloy grade and measured composition (including the share of returns)
- Pouring temperature and die temperature (heat-balanced, not first shot)
- Slow shot speed and slow-shot share of the sleeve
- Fast-shot position and fast shot speed
- Gate velocity, with the gate area used for the conversion
- Intensification pressure and build-up time
- Dwell time and spray cycle
- Total overflow volume, vent depth, cleaning frequency
Those eight, plus an X-ray film or a pressure-test record, are what makes a trial reproducible. Without them, "it worked last time" stays a guess.
Four common mistakes
- Quoting plunger speed only. Same plunger speed with a different gate area gives fill velocities two times apart, and the comparison means nothing.
- Using pressure to cure all shrinkage. Pressure compacts shrinkage porosity; it cannot remove gas already folded into the metal. That needs sleeve fill, venting and vacuum.
- Copying first-shot settings into production. The first shot runs on a cold die and an unwarmed machine, so settings are usually too aggressive; copied over, they flash or stick.
- Cutting dwell to chase cycle time. The seconds saved are smaller than the rework from distortion and ejection cracks — and cracks often surface after machining, where they cost more.
FAQ
The ranges above differ a lot from what our supplier uses. Who is wrong?
Check the definition first: is the pressure "casting pressure after intensification" or "shot cylinder pressure"; is gate velocity a converted value or plunger speed; is die temperature a thermocouple reading or an infrared surface reading? Different definitions differ by more than a factor of two. Once the definitions match, argue about whether the value leaves the range.
Why does the same part need retuning on another machine?
Tonnage, sleeve diameter, accumulator condition and shot-end state all differ, so the actual gate velocity and build-up time change at identical settings. After a move, recalibrate fast-shot speed, intensification and sleeve fill.
For thin walls, is faster always better?
No. It has to be fast enough to avoid cold shuts, but past that point it entrains air and washes the die out. The test is whether fill time matches venting capacity: with inadequate vents, more speed only breaks the gas into finer bubbles that stay in the casting.
If the parameters are right, is the cost low?
Not necessarily. Parameters move machine time, die life and yield; alloy price, part weight, secondary operations and tooling are separate lines. A real should-cost fills all of them into the calculator rather than admiring one well-tuned number.
Related: die casting cost calculator · tonnage and sleeve fill · die casting mould cost · die casting defect checklist · process selection guide · glossary
References
- Product Standards for Die Castings NADCA · NADCA #401
- Castings — General dimensional and geometrical tolerances and machining allowances ISO · ISO 8062-3
Basis for the parameters above. Links go to the publisher or its search page; the standard text itself is sold by the publisher. Price references are public market ranges, not supplier quotations.