Injection molding quotes rarely stall because the arithmetic is wrong; they stall because nobody can say what parameters the part should run at. This page puts the four parameter families side by side — melt and mold temperature, injection and packing, resin drying, cooling and cycle — each with a working range and the defects you get outside it, so a trial report saying "silver streaks", "sinks" or "stress whitening" can be read as "the profile is not dialled in" or "this tool and resin cannot do it".

Ranges move with grade, wall thickness, machine and tool structure. The values below are common starting points in the industry, not clauses of a standard; the final numbers come from a documented trial. The references at the foot of the page cover molding process baselines and cycle estimation — they are not the basis for the temperatures and pressures above.

1. Melt and mold temperature: eight common plastics

Melt temperature sets how fluid the resin is; mold temperature sets how fast it cools and how crystallisation and orientation develop. Neither is "higher is better": too hot a melt degrades the polymer (POM, PC and PA66 are unforgiving, and degradation is irreversible), too hot a mold costs cycle time and sticks. Too cold a melt gives weak weld lines and molded-in stress; too cold a mold loses control of shrinkage and warpage.

MaterialMelt temperatureMold temperatureBelow the rangeAbove the rangeShop-floor note
ABS 200–240 °C 40–70 °C Visible weld lines, poor flow, high molded-in stress Distortion after ejection, longer cycle, oversized parts Below 200 °C, silver streaks are usually blamed on wet resin
PP 200–260 °C 30–60 °C Uneven shrinkage, flow marks, weak weld lines Shrinkage grows further, warpage, longer cycle PP shrinks 1.5%–2.5%; mold temperature controls dimensional stability
PE 170–230 °C 20–50 °C Weak weld lines, rough surface Warpage, continued shrinkage after ejection HDPE and LDPE sit in different bands — go by grade
PS 180–240 °C 20–60 °C High stress, easy cracking Longer cycle, more flash risk GPPS runs at the top of the band, HIPS lower
PMMA 210–250 °C 40–80 °C Flow marks, haze in clear parts Sticking, yellowing from degradation, bubbles Clear parts below 40 °C mold temperature haze up visibly
PC 270–320 °C 80–110 °C Stress cracking, stress marks in clear parts Yellowing, sticking, stringing at the sprue Must be dried; do not compensate for low melt temperature with residence time
POM 190–210 °C 80–100 °C Porous surface, weak weld lines Formaldehyde smell, corrosion of the mold face Narrow window — decomposition starts above 220 °C
PA66 270–300 °C 70–110 °C Short shots, weak weld lines Warpage, hydrolytic degradation (worse if wet) Picks up moisture fast; use it from a sealed hopper

The materials above are the same eight, in the same order, as the built-in list in the injection molding cost calculator. If the resin has not been chosen yet, run the plastic material selector against budget and service temperature first, then come back for the parameter row. Melt and mold temperature also drive cooling time, which the cycle time calculator converts.

2. Injection and packing: set the transfer point before adding pressure

Injection pressure only has to fill the cavity; packing pressure is what compensates shrinkage. Shops blend the two, so a sink gets answered with more injection pressure and the result is flash plus molded-in stress with the sink still there. The order is: set the transfer point so filling does not overshoot, then fix compensation with packing pressure and packing time.

ParameterWorking rangeWhat it doesOutside the rangeHow to set it
Injection pressure 80–200 MPa (typical parts 100–140) Pushes the melt through and fills the cavity in the filling stage Too high: flash, molded-in stress, die wear; too low: short shots, missing corners, deep weld lines Take the top for thin walls, long flow and cold molds; fill first, then talk about appearance
Packing pressure 30%–70% of injection pressure Compensates shrinkage as the melt cools Too high: flash, stress whitening at ejectors, hard ejection; too low: sinks, voids, undersized parts Set it where sinks disappear near the gate; never use packing to rescue a gate that is too small
Packing time 3–10 s, set by gate freeze Keeps feeding material until the gate seals Too short: feeding stops early, sinks and dimensional drift; too long: longer cycle, higher stress Weigh parts while increasing packing until part weight stops rising
Transfer point (V/P) 95%–99% of stroke, or pressure/time based Switches from velocity control to pressure control, deciding whether filling overshoots Too late: the cavity is full but injection continues at speed — flash and stress; too early: short shots Position transfer is most common; thin walls transfer on pressure more reliably
Back pressure 0.3–1.0 MPa (higher for colour masterbatch and mixing) Compacts the melt and vents gas off the screw Too high: melt overheats and degrades, longer recovery; too low: air intake, black specks, poor colour mixing Raise it for clear and coloured parts, run the low end elsewhere to save energy

Injection pressure and clamp force are a pair: as cavity pressure rises, so does the force trying to open the mold, and a machine that is too small flashes. Check capacity with the clamp force and tonnage calculator rather than "running a shot to see" — once flash is pressed out, the parting line has already started to suffer.

3. Drying: the most commonly skipped step

More than half of the silver streaks, bubbles and lost mechanical properties on hygroscopic resins come from insufficient drying, not from a bad profile. The awkward part is that it drifts: resin in the hopper picks up moisture through the shift, so the same settings pass in the morning and streak in the afternoon. When that happens, suspect the resin before the machine.

Hygroscopic classMaterialsDrying conditionsIf it is not dryShop-floor note
Non-hygroscopic PS / PP / PE Normally no drying needed Without drying: surface silver streaks from degradation or shear, not water Hopper at 70–80 °C is enough to stop condensation
Slightly hygroscopic ABS / PMMA 80 °C / 2–4 h Undried: silver streaks, bubbles, reduced clarity Regrind absorbs faster — dry it again when the regrind share is high
Highly hygroscopic PC 120 °C / 4–6 h, dew point below −20 °C Hydrolysis: impact strength collapses, yellowing, bubbles PC hydrolysis is irreversible — drying cannot fix resin that has already degraded
Very highly hygroscopic PA66 80–100 °C / 4–6 h (vacuum drying is faster) Viscosity drops, stringing, bubbles, mechanical properties fall sharply Use it from a sealed hopper; a few tens of minutes in shop air is enough to reabsorb moisture
How to tell — Weight-loss method or a moisture analyser Above spec, identical settings give good and bad parts in the same shift Watch whether silver streaks follow hopper residence time — the cheapest test there is

Dryer capacity is usually overestimated: a unit rated at 120 °C often never brings the resin to the set point, especially with low airflow and a full hopper. Measure resin temperature and dew point, not the number on the panel.

4. Cooling and cycle: the cycle is the machine cost

Cooling takes more than half of a typical cycle, and cooling time scales with wall thickness squared — double the wall and cooling roughly quadruples. That is why thinning walls is the first cost lever in molding, and why a quote should be questioned on wall thickness before resin price.

ParameterWorking rangeWhat it doesWhat drifting costsHow to set it
Cooling time Dominated by wall thickness squared: 2 mm ABS ≈ 8 s, 3 mm ≈ 18 s From end of packing to mold opening Too short: stress whitening, distortion, undersized parts; too long: longer cycle — machine cost rises directly Calculate it from wall, melt and mold temperature in the cycle time calculator; do not trim seconds by feel
Open/close and ejection 1–4 s Machine motion, set by mold structure and automation Long times usually come from lifters, slides and robot paths This part barely changes with cavity count, which is why multi-cavity tools amortise better
Total cycle 12–40 s for typical parts Cooling + mold motion + injection and packing Every 20% of cycle adds about 20% of machine cost — almost linear The most sensitive line in molding cost, and the biggest payoff from thinning walls
Mold temperature control ±2–5 °C (tighter for engineering parts) Keeps shrinkage and appearance consistent lot to lot Large swings: dimensional drift between lots, settings stop being reproducible Run one TCU per circuit group, not one unit across several loops

Do not trim cooling by feel: 2 mm versus 3 mm is 8 s versus 18 s, and on a machine costing 60 CNY/hour that moves unit machine cost from 0.21 to 0.38. The molding cycle calculator converts wall thickness, melt, mold and ejection temperature into cooling time; the result belongs on the machine-time line of the cost calculator.

Why these ranges are only a starting point

The same settings behave differently on another machine: screw diameter, L/D ratio, check-ring condition and aged heater bands all change the measured melt temperature, easily by 15 °C. A new resin lot changes it again, because regrind share, masterbatch and fillers move viscosity and crystallisation. Treating ranges as an acceptance standard is guaranteed to start an argument.

Use them as a question list instead. Faced with a trial report, ask for measured melt temperature, mold temperature, injection and packing pressure, packing time and drying conditions. A supplier who cannot answer those rarely holds consistency in production either.

How parameters become cost

In other words, parameters are not an internal shop-floor matter: they set machine time, yield and secondary work at the same time. In a negotiation, "this part is difficult" can be tested by asking for the numbers above and seeing which one genuinely leaves the range.

The nine numbers to request at a trial

  1. Resin grade, regrind share and measured moisture content
  2. Measured melt temperature (not the set point) and mold temperature per circuit group
  3. Injection pressure, packing pressure and packing time
  4. Transfer mode (position / pressure / time) and the transfer point
  5. Back pressure and screw speed
  6. Cooling time and total cycle
  7. Dryer model, drying temperature, drying time and dew point
  8. Cavity count and gate type, including hot-runner zone temperatures
  9. First-article dimensional report and the appearance standard (which face is the A surface)

Those nine, plus a first-article report, are what makes a trial reproducible. Without them, "it worked last time" stays a guess.

Four common mistakes

  1. Answering sinks with injection pressure. Sinks are a compensation problem — packing pressure and packing time. More injection pressure buys flash first and parting-line damage second.
  2. Calling every silver streak "wet resin". Shear streaks, degradation streaks and moisture streaks look alike. The test is what they follow: only moisture follows hopper residence time.
  3. Cutting cooling time to chase cycle. The seconds come back as stress whitening, distortion and out-of-tolerance dimensions — often discovered at assembly, where they cost more.
  4. Reporting set points, not measurements. Aged heater bands, thermocouple placement and TCU flow put measured values more than ten degrees away. Comparing two set-point sheets compares nothing.

FAQ

The mold temperature band is wide — which end should we use?

Three constraints decide it: appearance (hotter molds hide weld lines and flow marks), dimensions (hotter molds shrink more fully, leaving less post-shrinkage) and cycle (hotter molds cool more slowly). When they conflict, hold the dimensional and appearance requirements, then price the cycle penalty in the calculator.

Does PC really need drying, or is a heated hopper enough?

A heated hopper is not enough. PC hydrolyses in the melt, breaking molecular chains irreversibly; the symptom is a collapse in impact strength, and the part can look perfectly normal. Check drying records before touching the profile.

If the controller says 240 °C, is the melt at 240 °C?

No. That is the target for the heater bands. Measured melt temperature depends on screw speed, back pressure, residence time and shot size — only a purge test or a probe tells you. Continuous running and intermittent running differ by more than 10 °C.

If the parameters are right, is the cost low?

Not necessarily. Parameters move cycle, yield and secondary work; resin price, part weight, cavity count and tooling are separate lines. A real should-cost fills all of them into the calculator rather than admiring one well-tuned number.

Related: injection molding cost calculator · molding cycle time · clamp force and tonnage · plastic material selector · injection defect checklist · machine hour rate · glossary

References

  1. Injection Molding Handbook Hanser · ISBN 978-1-56990-400-1
  2. Plastics — Injection moulding of test specimens of thermoplastic materials ISO · ISO 294

Basis for the parameters above. Links go to the publisher or its search page; the standard text itself is sold by the publisher. Price references are public market ranges, not supplier quotations.